发送传真
X10CrAlSi13 X10CrAl13 1.4724
|
类 |
钢种Type |
化学成分(%)Chemical Composition(%) |
机械性能 Mechanical properties | |||||||||||
|
KS (JIS) |
ZPSS |
C |
Cr |
Ni |
Mo |
其它Others |
热处理条件Heat Treatment |
屈服强度(N/mm2) Yield strength |
抗拉强度 Tensile strength |
延伸率(%) Elongation |
硬度 Hardness | |||
|
HB |
HRB |
HV | ||||||||||||
|
奥氏体AUSTENITE |
301 |
301 |
≤0.15 |
16.0~18.0 |
6.00~8.00 |
- |
- |
S |
≥205 |
≥520 |
≥40 |
≤207 |
≤95 |
≤218 |
|
301L |
301L |
≤0.030 |
16.0~18.0 |
6.00~8.00 |
- |
N≤0.20 |
S |
≥215 |
≥550 |
≥45 |
≤187 |
≤90 |
≤200 | |
|
304 |
304 |
≤0.08 |
18.0~20.0 |
8.00~10.50 |
- |
- |
S |
≥205 |
≥520 |
≥40 |
≤187 |
≤90 |
≤200 | |
|
304J1 |
304Cu |
0.02~0.05 |
16.5~17.1 |
7.5~7.9 |
- |
Cu1.9~2.2 |
S |
≥155 |
≥450 |
≥40 |
≤187 |
≤90 |
≤200 | |
|
304L |
304L |
≤0.030 |
18.0~20.0 |
9.00~13.00 |
- |
- |
S |
≥175 |
≥480 |
≥40 |
≤187 |
≤90 |
≤200 | |
|
304N1 |
304N1 |
≤0.08 |
18.0~20.0 |
7.00~10.50 |
- |
N0.10~0.25 |
S |
≥275 |
≥550 |
≥35 |
≤217 |
≤95 |
≤220 | |
|
304N2 |
304N2 |
≤0.08 |
18.0~20.0 |
7.50~10.50 |
- |
Nb≤0.15 |
S |
≥345 |
≥690 |
≥35 |
≤248 |
≤100 |
≤260 | |